The process of recovering silver technology from waste silver catalyst by fire smelting was studied. CaO-Al2O3 binary slag system was formed by adding the slagging elements of calcium oxide, when the amount of calcium oxide is 7 kg, melting temperature of 1500℃, time is 6 h, the recovery rate of silver more than 98%; the specific gravity of silver is bigger, sink the bottom of crucible, slag phase and the metal phase separation, obtain high purity of silver more than 99.98%. |